Table 3 Physical properties of pseudostem fiber extracted from Nendran banana

From: Biosoftening of banana pseudostem fiber using cellulase and pectinase enzyme isolated from Aspergillus niger for textile industry

Sl. no

Property

Untreated fiber

Enzyme-treated fiber

2 h

4 h

24 h

48 h

1

Tensile strength (g/tex)

26.29 ± 0.04

26.12 ± 0.02

26.01 ± 0.04

23.12 ± 0.01

20.14 ± 0.03

2

Breaking load (g)

315.41 ± 0.02

314.05 ± 0.02

313.44 ± 0.02

310.07 ± 0.02

308.23 ± 0.02

3

Breaking extension (%)

1.88 ± 0.03

1.68 ± 0.01

1.47 ± 0.02

0.95 ± 0.01

0.85 ± 0.01

4

Tenacity (g/tex)

12.05 ± 0.02

11.88 ± 0.02

11.11 ± 0.01

10.71 ± 0.05

9.92 ± 0.03

5

Diameter (mm)

0.13 ± 0.01

0.13 ± 0.01

0.13 ± 0.01

0.12 ± 0.01

0.12 ± 0.01